PEI 美國基礎創(chuàng)新 ULTEM? Resin 1010P

| 物理性能 | 額定值 | 單位制 | 測試方法 |
密度 / 比重 | 1.27 | g/cm3 | ASTM D792,ISO 1183 |
熔流率(熔體流動速率)(337°C/6.6 kg) | 18 | g/10 min | ASTM D1238 |
熔融體積流量(MVR) | ISO 1133 | ||
340°C/5.0 kg | 13 | cm3/10min | |
360°C/5.0 kg | 25 | cm3/10min | |
吸水率 | |||
24 hr, 23°C | 0.25 | % | ASTM D570,ISO 62 |
飽和, 23°C | 1.3 | % | ASTM D570,ISO 62 |
平衡, 23°C, 50% RH1 | 0.20 | % | ISO 62 |
平衡, 23°C, 50% RH | 0.70 | % | ISO 62 |
| 硬度 | 額定值 | 單位制 | 測試方法 |
洛氏硬度 | |||
M 級 | 109 | ASTM D785 | |
M 計秤 | 106 | ISO 2039-2 | |
球壓硬度(H 358/30) | 140 | MPa | ISO 2039-1 |
| 機械性能 | 額定值 | 單位制 | 測試方法 |
拉伸模量 | |||
--2 | 3350 | MPa | ASTM D638 |
-- | 3200 | MPa | ISO 527-1/1 |
抗張強度 | |||
屈服3 | 115 | MPa | ASTM D638 |
屈服4 | 110 | MPa | ASTM D638 |
屈服 | 110 | MPa | ISO 527-2/50 |
伸長率 | |||
屈服4 | 7.0 | % | ASTM D638 |
屈服3 | 7.0 | % | ASTM D638 |
屈服 | 6.0 | % | ISO 527-2/50 |
斷裂4 | 60 | % | ASTM D638 |
斷裂3 | 60 | % | ASTM D638 |
斷裂 | 50 | % | ISO 527-2/50 |
彎曲模量 | |||
50.0 mm 跨距5 | 3200 | MPa | ASTM D790 |
100 mm 跨距6 | 3400 | MPa | ASTM D790 |
--7 | 3300 | MPa | ISO 178 |
彎曲應力 | |||
--7,8 | 160 | MPa | ISO 178 |
屈服, 50.0 mm 跨距5 | 165 | MPa | ASTM D790 |
屈服, 100 mm 跨距6 | 160 | MPa | ASTM D790 |
泊松比 | 0.36 | ASTM E132 | |
泰伯耐磨性(1000 Cycles, 1000 g, CS-17 轉輪) | 10.0 | mg | ASTM D1044 |
| 沖擊性能 | 額定值 | 單位制 | 測試方法 |
簡支梁缺口沖擊強度9 | ISO 179/1eA | ||
-30°C | 4.0 | kJ/m2 | |
23°C | 4.0 | kJ/m2 | |
懸壁梁缺口沖擊強度 | |||
-30°C | 41 | J/m | ASTM D256 |
23°C | 32 | J/m | ASTM D256 |
-30°C10 | 5.0 | kJ/m2 | ISO 180/1A |
23°C10 | 5.0 | kJ/m2 | ISO 180/1A |
無缺口懸臂梁沖擊 | |||
-30°C | 1500 | J/m | ASTM D4812 |
23°C | 1600 | J/m | ASTM D4812 |
-30°C10 | 無斷裂 | ISO 180/1U | |
23°C10 | 無斷裂 | ISO 180/1U | |
反向缺口沖擊(3.20 mm) | 1200 | J/m | ASTM D256 |
落錘沖擊(23°C) | 33.0 | J | 內部方法 |
| 熱性能 | 額定值 | 單位制 | 測試方法 |
載荷下熱變形溫度 | |||
0.45 MPa, 未退火, 3.20 mm | 207 | °C | ASTM D648 |
0.45 MPa, 未退火, 6.40 mm | 210 | °C | ASTM D648 |
0.45 MPa, 未退火, 4.00 mm, 64.0 mm 跨距10 | 209 | °C | ISO 75-2/Bf |
1.8 MPa, 未退火, 3.20 mm | 190 | °C | ASTM D648 |
1.8 MPa, 未退火, 6.40 mm | 201 | °C | ASTM D648 |
1.8 MPa, 未退火, 4.00 mm, 64.0 mm 跨距10 | 192 | °C | ISO 75-2/Af |
維卡軟化溫度 | |||
-- | 211 | °C | ASTM D152511,ISO 306/B5011 |
-- | 212 | °C | ISO 306/B120 |
-- | 215 | °C | ISO 306/A50 |
Ball Pressure Test(123 到 127°C) | 通過 | IEC 60695-10-2 | |
線形熱膨脹系數(shù) | |||
流動 : -20 到 150°C | 5.6E-5 | cm/cm/°C | ASTM E831 |
流動 : -20 到 150°C | 5.2E-5 | cm/cm/°C | ISO 11359-2 |
垂直 : -20 到 150°C | 5.4E-5 | cm/cm/°C | ASTM E831 |
垂直 : -20 到 150°C | 5.2E-5 | cm/cm/°C | ISO 11359-2 |
導熱系數(shù) | 0.22 | W/m/K | ASTM C177,ISO 8302 |
| 電氣性能 | 額定值 | 單位制 | 測試方法 |
表面電阻率 | 1.0E+15 | ohms | IEC 60093 |
體積電阻率 | |||
-- | 1.0E+17 | ohms·cm | ASTM D257 |
-- | 1.0E+15 | ohms·cm | IEC 60093 |
介電強度 | |||
1.60 mm, in Air | 33 | kV/mm | ASTM D149 |
1.60 mm, in Oil | 28 | kV/mm | ASTM D149 |
3.20 mm, in Oil | 20 | kV/mm | ASTM D149 |
0.800 mm, 在油中 | 33 | kV/mm | IEC 60243-1 |
1.60 mm, 在油中 | 25 | kV/mm | IEC 60243-1 |
3.20 mm, 在油中 | 16 | kV/mm | IEC 60243-1 |
介電常數(shù) | |||
100 Hz | 3.15 | ASTM D150 | |
1 kHz | 3.15 | ASTM D150 | |
1.10 GHz | 3.01 | 內部方法 | |
5.00 GHz | 3.02 | 內部方法 | |
10.0 GHz | 3.02 | 內部方法 | |
50 Hz | 2.90 | IEC 60250 | |
60 Hz | 2.90 | IEC 60250 | |
1 MHz | 2.90 | IEC 60250 | |
耗散因數(shù) | |||
100 Hz | 1.5E-3 | ASTM D150 | |
1 kHz | 1.2E-3 | ASTM D150 | |
1.10 GHz | 1.2E-3 | 內部方法 | |
5.00 GHz | 2.4E-3 | 內部方法 | |
10.0 GHz | 2.7E-3 | 內部方法 | |
50 Hz | 5.0E-4 | IEC 60250 | |
60 Hz | 5.0E-4 | IEC 60250 | |
1 MHz | 6.0E-3 | IEC 60250 | |
漏電起痕指數(shù) | IEC 60112 | ||
-- | 150 | V | |
解決方案 B | 100 | V | |
| 可燃性 | 額定值 | 單位制 | 測試方法 |
極限氧指數(shù) | 44 | % | ASTM D2863 |